Selective Laser Melting of Nickel Superalloys: Solidification, Microstructure and Material Response

Total Page:16

File Type:pdf, Size:1020Kb

Load more

Selective Laser Melting of Nickel Superalloys: solidification, microstructure and material response By: Neil J Harrison A thesis submitted in partial fulfilment of the requirements for the degree of Doctor of Philosophy The University of Sheffield Faculty of Engineering School (or Department) of Mechanical Engineering Submission Date: 28th of October 2016 Abstract The Selective Laser Melting (SLM) process generates large thermal gradients during rapid melting, and during solidification certain nickel superalloys suffer from thermally induced micro-cracking which cannot be eliminated by process optimisation. This investigation sought to investigate and understand the root cause of micro-cracking in nickel superalloys when processed by SLM, with the aim of ultimately being able to predict the crack susceptibility of an alloy from composition alone. Microstructural analysis as well as implementation of Rapid Solidification Processing (RSP) theory and solute redistribution theory was used to establish SLM as a rapid solidification process. As a consequence, secondary dendrite arm formation and solute redistribution is largely inhibited, resulting in a bulk material which is near to a super saturated solid solution. The establishment of SLM as an RSP along with morphological and chemical analysis of micro-cracks support Elevated Temperature Solid State (ETSS) cracking as the primary cracking mechanism in SLM processed nickel superalloys. The crack susceptibility of a nickel superalloy, χ, was defined as the ratio between the solid solution strengthening contribution from alloying elements and apparent thermal stress generated by the process. Minor increases in the wt% of solid solution strengthening elements in Hastelloy X, a high crack susceptibility alloy, resulted in average reductions of crack density of 65%. Thereby supporting solid solution strength as a key factor in the crack susceptibility of a nickel superalloy. The addition of the apparent thermal stress component, further supported 1 the crack susceptibility model, with the modified Hastelloy X being predicted to have a lower crack susceptibility. Additional validation of the crack susceptibility predictor was determined by taking compositions and material properties from published SLM investigations and calculating the crack susceptibility of the respective alloy. The results were found to be in good agreement with the reported observations. Acknowledgments I would like to thank everyone who has made success in this project possible. As with anything of this scale, there are countless people involved at various points, all of whom have had an effect on the process and outcome of the work. However, I feel it necessary to thank the following people specifically for their significant contributions and support: I would like to thank my primary academic supervisor, Dr Kamran Mumtaz, for his support and guidance throughout this project. His encouragement and knowledge of this field ensured a successful conclusion to this project, along with publication of part of this work in a high ranking journal. I would also like to thank my secondary supervisor, Professor Iain Todd, whose extensive knowledge of metallurgy and enthusiasm for the project was invaluable. I can attribute much of my learning regarding the fundamental aspects of this work to his guidance. I thank LPW Technology Ltd and EPSRC for their financial support in this project. I also wish to thank my industrial supervisor, Dr Robert Deffley, whose work provided the platform for this project and whose knowledge of the process and nickel alloys 2 specifically was also invaluable. In addition, I personally thank Dr Phil Carroll (CEO of LPW Technology) for his technical support and helping me integrate with the company. I would like to thank my colleague Omar Lopez, whose temperature field model featured in this work, in addition to his general support and imparting of knowledge in this area. Other colleagues without whose assistance I would not have be able to complete this work in its entirety are Dr James Hunt, Dr Fatos Derguti, Ian Woods, Kyle Arnold, Pratik Vora and Dr Cheryl Shaw. I would also like to thank the Departments of Mechanical Engineering and Materials Science and Engineering at the University of Sheffield for administrative support, use of equipment, and provision of courses and literature for personal development. The guys in D14 Garden Street also deserve significant praise for breaking up the long days with occasional games of office golf and various internet base games, but punctuated with actual work. Without them, I doubt I would have had the drive required to put in a full day every day. So thank you Tom, Ryan, Ste and Luke. Perhaps the greatest thanks goes to my family, without the support, encouragement and love from them, I would have struggled to get through the difficult periods of the last 4 years. Mum, Dad, Mark, Sue, Alastair, Grandma, I love you and thank you. Finally my beautiful wife, Catherine, thank yous will never be enough to balance the love, support and encouragement you have given me. Without you I would never have considered this avenue in my career, and therefore I would have never have found myself in the position that I am in now. From long before this project began, throughout its duration and every day after, you have been my constant, my rock, and my best friend. I could not have done this without you. I love you more than anything. 3 Table of Contents Abstract ................................................................................................................................................................................ 1 Acknowledgments ............................................................................................................................................................ 2 Table of Contents .............................................................................................................................................................. 4 Publications ........................................................................................................................................................................ 8 List of Tables ....................................................................................................................................................................... 8 List of Figures ..................................................................................................................................................................... 9 List of Abbreviations .................................................................................................................................................... 15 Nomenclature .................................................................................................................................................................. 17 1 Introduction ........................................................................................................................................................... 21 1.1 Problem statement .................................................................................................................................... 21 1.2 Aims and Objectives of Research ......................................................................................................... 22 1.3 Thesis structure .......................................................................................................................................... 22 2 Background and Literature review .............................................................................................................. 25 2.1 Selective Laser Melting: An Additive Manufacturing technique ............................................. 25 2.1.1 The process ......................................................................................................................................... 25 2.1.2 Applications ........................................................................................................................................ 27 2.2 Problem characteristics in SLM ............................................................................................................ 29 2.2.1 High thermal and residual stresses ........................................................................................... 29 2.2.2 Porosity ................................................................................................................................................. 37 2.2.3 Surface roughness ............................................................................................................................ 39 2.2.4 Process induced cracking .............................................................................................................. 42 2.3 Failure by fracture and critical crack length ................................................................................... 44 2.4 Solidification and microstructure theory ......................................................................................... 47 2.4.1 Solidification fundamentals.......................................................................................................... 47 2.4.2 Rapid solidification .......................................................................................................................... 55 2.4.3 In SLM ...................................................................................................................................................
Recommended publications
  • Role of Cobalt in Waspaloy

    Role of Cobalt in Waspaloy

    ROLE OF COBALT IN WASPALOY G. E. Maurer L. A. Jackman J. A. Domingue Special Metals Corp., New Hartford, N.Y. 13413 Nickel was systematically substituted for cobalt in Was- paloy. M'echanical test results indicate that lower cobalt has little effect on tensile properties, but adversely affects creep rate and stress rupture life. Phase extraction studies found slight decreases in gamma prime volume fractions and in- creased M'23C6 carbide with lowes cobalt. It is suggested that changes in gamma prime volume fraction, carbide precipitation, and stacking fault energy contribute to the decrease in creep resistance. INTRODUCTION Interest in the role of specific elements in the design of nickel-base superalloys has been dramatically revitalized in the past two years. Economic and strategic considera- tions have prompted re-examination of the necessity of raw materials whose availability could be jeopardized by political unrest or resource depletion. Recently, an ele- ment of primary concern has been cobalt, which comprises from 8-19 wt.% of some of the most commonly used wrought alloys. Information on the role of cobalt in nickel-base super- alloys was found insufficient to ascertain if the specified levels of cobalt in many commercial superalloys is justi- fied. Therefore, a one variable study was initiated on the systematic replacement of cobalt by nickel in Waspaloy, which accounts for the greatest consumption of "nickel- base superalloy" cobalt. Few studies have been done on the specific reduction of cobalt in a superalloy cl.-3). The principle reference to the overall role of cobalt in wrought superalloys is by Heslop (1) who reviewed the use 43 44 / Superalloys 1980 of cobalt in Nimonic alloys.
  • Weld Cracking of Precipitation Hardening Ni-Based Superalloys

    Weld Cracking of Precipitation Hardening Ni-Based Superalloys

    THESIS FOR THE DEGREE OF DOCTOR OF PHILOSOPHY Weld Cracking of Precipitation Hardening Ni-based Superalloys Investigation of repair welding characteristics and susceptibility towards strain age cracking Fabian Hanning Department of Industrial and Materials Science CHALMERS UNIVERSITY OF TECHNOLOGY Gothenburg, Sweden i Weld Cracking of Precipitation Hardening Ni-based Superalloys Investigation of repair welding characteristics and susceptibility towards strain age cracking Fabian Hanning ISBN 978-91-7905-258-4 © Fabian Hanning, 2020 Doktorsavhandlingar vid Chalmers tekniska högskola Ny serie nr 4725 ISSN 0346-718X Department of Industrial and Materials Science Chalmers University of Technology SE-412 96 Gothenburg Sweden Telephone + 46 (0)31-772 1000 Printed by Chalmers digitaltryck Gothenburg, Sweden 2020 ii Weld Cracking of Precipitation Hardening Ni-based Superalloys Investigation of repair welding characteristics and susceptibility towards strain age cracking Fabian Hanning Department of Industrial and Materials Science Chalmers University of Technology Abstract High temperature resistance and strength requirements make nickel-based superalloys the material of choice for the hot section of aero engines. Fabrication in terms of combining wrought and cast parts in the manufacturing of hot structural components enables component optimisation via the use of wrought high-strength parts, where geometrical constraints allow, and cast parts to produce complex geometries. Such an approach requires that the materials involved are weldable. Due to the complex microstructure of precipitation hardening nickel-based superalloys, welding comes with the risk of weld cracking, more specifically solidification cracking, heat affected zone (HAZ) liquation cracking and strain age cracking (SAC). While the first two types require a liquid phase to be present, SAC occurs during heating to post-weld heat treatment, in which age-hardening reactions coincide with the relaxation of weld residual stresses.
  • Capabilities of Midlands Aerospace Companies 2016

    Capabilities of Midlands Aerospace Companies 2016

    midlands aerospace alliance Capabilities of Midlands Aerospace Companies 2016 - 2017 Midlands capability for the world’s aerospace industry he Midlands Aerospace Alliance is pleased to present you with the updated 2016-17 edition of our Tmember capability directory – which marks our eleventh annual edition. It has been designed to help you identify world-class Midlands partners and suppliers for your aerospace programmes and projects. The Midlands is home to one of the largest aerospace clusters in the world. Aerospace technologies designed and made in the Midlands can be found on the world’s most advanced aircraft. Leading names such as Rolls- Royce Controls and Data Services, Meggitt, Moog, Rolls-Royce and UTC Aerospace Systems are major players in a region renowned for its core competency technologies: • systems that power aircraft – gas turbine engines and other propulsion systems • systems that control the moving parts of aircraft and engines – electrical, mechanical, electronic, hydraulic and pneumatic • specialist metal and composite materials that enable these systems to perform with precision in exacting Contents environments • specialist engineering design services, factory equipment and tooling. The Midlands business environment fosters the highest levels of innovation. Aerospace supply chains extend deep into our cluster’s world-class advanced engineering economy. We access and invest in a dynamic skills base, with more than 45,000 skilled people working in our aerospace industry. The mission of the Midlands Aerospace Alliance is to enhance cooperation between customers, suppliers and partners in the Midlands and globally, so that we can improve the performance of all our companies and organisations. We invite you to join us, using this directory to identify the new partners and suppliers you need to make your projects successful.
  • Haynes® 282® Alloy

    Haynes® 282® Alloy

    HIGH-TEMPERATURE ALLOYS HAYNES® 282® ALLOY A new, wrought, age-hardenable, nickel superalloy designed for improved creep strength, weldability, and fabricability. Contents Principal Features 3 Creep and Stress-Rupture Strength 4 Strain-Age Cracking Resistance 7 Tensile Properties 8 Hardness 9 Aging Kinetics 10 Oxidation Resistance 11 Thermal Stability 13 Physical Properties 15 Low Cycle Fatigue 17 Welding 18 Heat Treatment and Fabrication 22 Health and Safety 25 Service Center Information 27 H-3173 TYPICAL APPLICATIONS HAYNES® 282® alloy is designed for applications in engines for aircraft. HAYNES® 282® alloy is designed for the transition sections and other hot-gas-path components in land-based gas turbines. HAYNES® 282® alloy 2 ©2008 Haynes International, Inc. PRINCIPAL FEATURES Excellent High Temperature Strength HAYNES® 282® alloy is a new, wrought, gamma-prime strengthened superalloy developed for high temperature structural applications, especially those in aero and land-based gas turbine engines. It possesses a unique combination of creep strength, thermal stability, weldability, and fabricability not found in currently available commercial alloys. The new alloy has excellent creep strength in the temperature range of 1200 to 1700°F (649 to 927°C), surpassing that of Waspaloy alloy, and approaching that of R-41 alloy. Easily Fabricated This high level of creep strength in HAYNES 282 alloy has been attained at a relatively low volume fraction of the strengthening gamma-prime phase, resulting in outstanding resistance to strain-age cracking (normally a problem with superalloys in this creep strength range). Additionally, slow gamma-prime precipitation kinetics allow for the alloy to have excellent ductility in the as-annealed condition.
  • Gas Turbine Superalloy

    Gas Turbine Superalloy

    GAS TURBINE SUPERALLOY WITH IMPROVED FABRICABILITY A wrought gamma-prime strengthened superalloy combines high-temperature strength with excellent formability for gas turbine engine components. Lee M. Pike* H. Lee Flower* Haynes International Kokomo, Indiana new wrought nickel-chromium-cobalt- molybdenum superalloy, designated Haynes 282 alloy, possesses a unique combination The Haynes 282 alloy is designed for applications in engines for aircraft such of high-temperature strength and fabri- as the Lockheed Martin F-35 Joint Strike Fighter. cability that gives it a distinct advantage Aover other alloys. The attributes of the alloy are cracking. On the other hand, higher levels of well suited for a wide variety of high-tempera- gamma-prime are beneficial for high-tempera- ture applications, particularly those in aero and ture strength. Therefore, the gamma-prime con- land-based gas turbine engines. tent is balanced so that 282 alloy is easy to fabri- With 57% nickel, 20% chromium, 10% cobalt, cate, yet still possesses excellent creep strength. and 8.5% molybdenum (Table 1), the alloy falls The features of 282 alloy make it suitable for into a subcategory within the larger category of critical applications such as sheet fabrications and the familiar gamma-prime-strengthened super- seamless and flash butt-welded rings found in alloys. This subcategory includes such alloys as compressor, combustor, and turbine sections. In Waspaloy, René-41 (or R-41), and 263, which are augmented aircraft gas turbines, the new alloy distinguished by their ability to be produced as will be useful for exhaust and nozzle components. flat products; that is, in the form of hot-rolled plate In land-based gas turbines, 282 alloy is a good op- and/or cold-rolled sheet.
  • The of Metal With

    The of Metal With

    / NASA _Technical _r Paper d 3128 August 1991 The _n of With Metal . - L - _ = L : __-___.....;-'.__ ,-- _ _ L ..... .7 _ .... r m ___ ;.. _-_ .-) _-: 2 . ,, c .... - _.- . • . ! -/ • - . -. , . -. ,! - y÷. .... -_" r i. .2 .- .... " - _ L _. _ _" _-- - .-- _ -" "; "7 NASA Technical Paper 3128 1991 The Interaction of Hydrogen With Metal Alloys M. D. Danford and J. W. Montano George C. Marshall Space Flight Center Marshall Space Flight Center, Alabama National Aeronautics and Space Administration Office of Management Scientific and Technical Information Program TABLE OF CONTENTS Page INTROI)UCTION .............................................................................................. I EXPERIMENTAL .............................................................................................. I RESULTS AND DISCUSSION .............................................................................. Crystal Structure ....................................................................................... ,3 Diffusion Coefficients ................................................................................. 3 Hydrogen Desorption Curves ........................................................................ 3 The Role of Hydride Formation in Hydrogen kimbrittlen_ent .................................... 4 Relation of Structure to Hydrogen Distribution on Charging .................................... 4 The Correlation of Structure and Composition With Notched Ten si le Stren,,th 5 CONCLUSIONS ...............................................................................................
  • NASA Contractor Report 174628 the Role of Cobalt on the Creep Of

    NASA Contractor Report 174628 the Role of Cobalt on the Creep Of

    NASA Contractor Report 174628 The Role of Cobalt on the Creep of Waspaloy Robert N. Jarrett, Lori Chin, and John K. Tien Columbia University New York, New York February 1984 Prepared for NATIONAL AERONAUTICS AND SPACE ADMINISTRATION Lewis Research Center Under Grant NAG3-57 Trade names or manufacturers’ names are used in this report for identification only. This usage docs not constitute an official endorsement, either expressed or implied, by the National Aeronautics and Space Administration. 1 As part of the NASA Conservation of Strategic Aerospace Materials (COSAIG) programlD2 we have studied the role of cobalt variations on the static properties of Waspaloy. Previously, we reported the effects of cobalt on Udimet TOO3? A comparitive study on Waspaloy is interesting since this alloy has the same alloying elements as Udimet 700, except that Waspaloy has less aluminum and titanium (and hence, less 7' precipitates) and less molybdenum for solid solution strengthening, For these reasons Waspaloy belongs to a lower strength class of alloys. In the study on Udimet 700, systematic creep and tensile tests were correlated with microstructure and microchemistry results to determine the effects of replacing cobalt with nickel in the alloy which normally contains 18% cobalt. These alloys were given a sub-solvus heat treatment used to retain some primary y* to pin grain boundaries. This fine grain material is designed for lower temperature, but higher strength applications--such as the gas turbine disk. The yield and tensile strengths of low cobalt Udimet 700 were found to be slightly lower than the standard alloy. This small decrease in tensile strength was attributed to th3 slight decrease in strengthening y' fraction even though the total 7' fraction was found to be independent of alloy cobalt content3,4s6 4 2 In contrast to the small effect of cobalt on tensile properties, creep and stress rupture strength of the low cobalt alloys fell drastically.
  • Superalloys, the Most Successful Alloy System of Modern Times-Past, Present, and Future

    Superalloys, the Most Successful Alloy System of Modern Times-Past, Present, and Future

    SUPERALLOYS, THE MOST SUCCESSFUL ALLOY SYSTEM OF MODERN TIMES - PAST, PRESENT AND FUTURE Art Kracke Vice President Business Technology ATI Allvac Abstract The deep roots of superalloys go back to 1907, although the term ‘super-alloy’ is believed to have first been used in the mid 1940s to refer to cobalt-base alloys such as Vitallium and nickel- base Waspaloy®. During the past 50 years, much alloy, hot working, heat treating and process development has occurred, enabling many of the end use technologies we know today. This presentation will discuss some of the history of the superalloy industry related to the superalloys 718, Waspaloy and their derivatives, including ATI 718Plus® alloy. The presentation will then describe the wide range of manufacturing techniques used for the production of superalloys, available product forms and end-use applications. Concluding the presentation will be a discussion on what advancements we are likely to see in the future. Introduction Superalloys are successful today because they have solved pressing demands for durability and strength in machines and systems that were barely imaginable a hundred years ago. Superalloys have helped us conquer air and space, plumb the depths of the earth and ocean, and address many other challenges of modern life. As such, they deserve to have their story told. The nature of this industry, however, makes the telling a challenging task. Its history is one of many small events and inventions that took place across the boundaries of nations, industries and countries. Many individuals contributed to the state of the art today, and only a few left their names in the scattered records.
  • AEROSPACE APPLICATIONS INDEX AEROSPACE AIR FRAME Y CFRP Y CFRP/AI Y CFRP/Ti Tool Page

    AEROSPACE APPLICATIONS INDEX AEROSPACE AIR FRAME Y CFRP Y CFRP/AI Y CFRP/Ti Tool Page

    A614G AEROSPACE APPLICATIONS INDEX AEROSPACE AIR FRAME y CFRP y CFRP/AI y CFRP/Ti Tool Page Drilling MCC Drill 5 Drilling MCA Drill 6 Trimming DFC End Mill 7 y Aluminium Alloy y Aluminium-lithium Alloy Face Milling, Pocket Milling AXD Series 8 Face Milling, Pocket Milling AXD Series 9 Face Milling, Pocket Milling ALIMASTER 10 Exchangeable Head End Mills Face Milling, Pocket Milling iMX Series 11 y Titanium Alloy Side Milling, Rough Pocket Milling VFX Series 12 Face Milling, Side Milling AJX Series 13 Side Milling, Pocket Milling ARP Series 14 VQT5MVRB Slotting Corner Radius End Mill for High Effi ciency Titanium Alloy Machining 15 Side Milling, Pocket Milling Coolstar Series 16 y Precipitation Hardening Stainless Steel Rough Pocket Milling VPX Series 17 Drilling MMS Drill 18 2 ENGINE y Ni-based Superalloy Tool Page LS/MJ/MS/MA/RS External, Face and Internal Turning MP9005/MP9015/MP9025 20 External, Face and Internal Turning US905/VP05RT/VP10RT 21 Copy Turning GY Series 22 Machining of Upper Surface of Protuberance APX Series 23 Drilling (Helical), Profi le Milling ARX/ARP Series 24 Drilling (Helical), Profi le Milling CERAMIC End Mill 25 SMART MIRACLE Finish Profi le Milling Vibration Control Ball Nose End Mill 26 VQT6UR Finish Profi le Milling Barrel End Mill for Finish Cutting of Titanium Alloys 27 Drilling MMS Drill 28 y Titanium-aluminium Alloy SMART MIRACLE Finish Profi le Milling End Mill Series 29 y Titanium Alloy External, Face and Internal Turning LS/MS/RS MT9005/MT9015 30 y Maraging Steel External, Face and Internal Turning FJ/MJ/MS/GJ
  • Aerospace — High-Temperature Machining Guide

    Aerospace — High-Temperature Machining Guide

    High-Temperature Machining Guide High-Temperature Machining Superalloys, also known as heat-resistant superalloys No material is perfect, however. Historically, one drawback or high-temperature alloys, are materials that can be of superalloys has been their poor machinability. This is machined at temperatures exceeding 1000˚ F (540˚ C). where Kennametal comes in. No other alloy system has a better combination of high- temperature corrosion resistance, oxidation resistance, Kennametal has decades of experience working with material and creep resistance. Because of these characteristics, providers, OEMs, and parts manufacturers, resulting in an superalloys are widely used in aircraft engine components unmatched portfolio of standard and custom solutions. We and in industrial gas turbine components for power are proud to be the supplier of choice in superalloy tooling generation. They are also utilized in petrochemical, solutions for most OEMs, and their subcontractors, around oil, and biomedical applications, specifically for the world. their excellent corrosion resistance. We would like to share with you some of this knowledge, Today, fuel efficiency and reliability drive modern aircraft and are pleased to present the following guide to machining engine design. Engineers have long relied upon superalloys, these materials. Topics covered range from understanding such as INCONEL® and Waspaloy™, for their unique high- metallurgical properties of superalloys to the best temperature and stress-resistance properties. Such technologies for machining. properties are especially critical to the aerospace industry. Modern aircraft engines are far more reliable than their predecessors, and thanks to great strides in technology, it is now common to “stay on wing” for years. These engines are also powerful and dependable enough that just two can power large jetliners across entire oceans without concern.
  • Court File No. CV-14-10573-00CL ONTARIO SUPERIOR

    Court File No. CV-14-10573-00CL ONTARIO SUPERIOR

    Court File No. CV-14-10573-00CL ONTARIO SUPERIOR COURT OF JUSTICE (COMMERCIAL LIST) IN THE MATTER OF THE COMPANIES' CREDITORS ARRANGEMENT ACT, R.S.C. 1985, c. C-36, AS AMENDED AND IN THE MATTER OF A PLAN OF COMPROMISE OR ARRANGEMENT OF KK PRECISION INC. Applicant MOTION RECORD (Returnable August 1, 2014) July 25, 2014 DENTONS CANADA LLP 77 King Street West, Suite 400 Toronto-Dominion Centre Toronto, ON M5K 0A1 John Salmas (LSUC 42336B) Tel: (416) 863-4374 Fax: (416) 863-4592 Email: john.salmas@dentons.com Robert J. Kennedy (LSUC 47407O) Tel: (416) 367-6756 Fax: (416) 863-4592 Email: robert.kennedy@dentons.com Solicitors for the Applicant 9780079_3|NATDOCS - 2 - SERVICE LIST TO: AIRD & BERLIS LLP Brookfield Place 181 Bay Street, Suite 1800 P.O. Box 754 Toronto, ON M5J 2T9 Steven L. Graff Telephone: (416) 865-7726 Fax: (416) 863-1515 Email: sgraff@airdberlis.com Ian Aversa Telephone: (416) 865-3082 Fax: (416) 863-1515 Email: iaversa@airdberlis.com Solicitors for Bank of Montreal and BMO Capital Corporation AND TO: MILLER & MARTIN PLLC Suite 1000 Volunteer Bldg. 832 Georgia Avenue Chattanooga, TN 37402 Jonathan F. Kent Telephone: (423) 785-8301 Fax: (423) 321-1539 Email: jkent@millermartin.com Solicitor for River VI, L.P. AND TO: CHAITON LLP 5000 Yonge Street 10th Floor Toronto, ON M2N 7E9 Sam Rappos Telephone: (416) 218-1137 Fax: (416) 1837 Email: samr@chaitons.com Solicitor for the Monitor AND TO: GOWLING LAFLEUR HENDERSON LLP 1 First Canadian Place 100 King Street West 9780079_3|NATDOCS - 3 - Suite 1600 Toronto, ON M5X 1G5 Frank Lamie Telephone: (416) 862-3609 Fax: (416) 862-7661 Email: frank.lamie@gowlings.com Solicitor for Siemens Energy Inc.
  • ATI Waspaloy* Alloy

    ATI Waspaloy* Alloy

    ATI Waspaloy* Alloy Technical Data Sheet ATI Waspaloy* Alloy INTRODUCTION The alloy is a high strength, nickel base, precipitation hardening alloy which gains its high strength through the precipitation of gamma prime as a result of titanium and aluminum additions and through solid solution strengthening from additions of chromium, cobalt, and molybdenum. Precipitated carbides provide additional strengthening by pinning grain boundaries which reduce grain boundary sliding at elevated temperatures. The alloy is used for critical parts that require high strength at elevated temperatures. It is produced by vacuum induction melting (VIM) followed by vacuum arc remelting (VAR) and/or electroslag remelting (ESR). Applications include turbine and compressor discs, shafts, spacers, turbine cases, fasteners and other miscellaneous hardware. Super Waspaloy alloy is a higher strength, thermo-mechanically processed grade that has slightly lower carbon content and higher titanium and aluminum contents. SPECIFICATIONS • AMS 5704 - Forgings: solution, stabilization, and precipitation heat treated • AMS 5706 - Forgings, bars, and rings: solution heat treated • AMS 5707 - Forgings, bars, and rings: solution, stabilization and precipitation heat treated • AMS 5708 - Forgings and bars: solution heat treated • AMS 5709 - Forgings and bars: solution, stabilization and precipitation heat treated PHYSICAL PROPERTIES Melting Range: 2,425 to 2,565 ºF (1,329 to 1,407 ºC) Density: 0.296 lbs/in3 (8.20 gm/cc) HEAT TREATMENT Solution treatment is at 1,825 to 1,900 0F (996 to 1,038 ºC), 4 hours, water or oil quench or 1,975 ºF (1,079 ºC), ½ or 4 hours, air cool. Stabilization treatment is 1,550 ºF (843 ºC), 4 or 24 hours, air cool.